Fracture mechanics · a guided exercise · about 45 minutes once you know the background
A bridged crack: when does the first connector fail?
Fibres or ligaments that bridge a crack hold its faces together. You will find the load at which the
first of them breaks, see why a toughness cannot give that load here, and then find the error in a formula that an AI
agent wrote for the same problem.
You will practice
deciding whether bridging can be condensed into a toughness;
coupling a bridging law to a finite crack through two conditions;
choosing a check that can actually catch a wrong formula.
You need
the stress intensity factor and superposition of crack-face loads;
the strip-yield (Dugdale) crack;
pen and paper, and something to solve one equation numerically.
New to fracture mechanics? Start with Fracture Mechanics 101; each step below links to the topic it needs.
1 The problem
A large plate in plane strain contains a slit of half-length a. A remote tension Σ pulls it open.
As the load rises the crack grows at both ends, and connectors stay behind across the new crack faces, over a
length L at each end. Each connector pulls the faces together with a constant traction
σb until the gap between the faces reaches δc; then it breaks for
good. Moving the crack front itself costs a work Γ0 per unit area, separate from the
connectors.
Half-length of the slit
a
2.40 mm
Young’s modulus, Poisson’s ratio
E, ν
130 GPa, 0.28
Connector traction
σb
160 MPa
Gap at which a connector breaks
δc
9.00 µm (full gap, face to face)
Work to advance the front
Γ0
22.0 J/m²
Find the remote stress Σ at which the first connector breaks (the one next to the original slit),
and the bridged length L at each end at that moment.
Try it on paper first. An answer counts as right within 0.3%, the tolerance the AI agents were
given. If you get stuck, the steps below take you there.
The task exactly as the AI agents received it
A finite flaw under opening tension. An infinite isotropic plate in plane strain contains a straight, traction-free slit on y = 0,
from x = −a to x = a, with a = 2.40 mm.
A uniform remote tensile stress Σ acts normal to the slit. The solid has E = 130 GPa, ν = 0.28.
As the two crack fronts advance along the slit line, intact connectors remain between the separated faces on
a < |x| < a + L. Their closing normal traction under
monotonic opening is t(δ) = 160 MPa (0 < δ < 9.00 µm),
and becomes zero irreversibly when the opening first reaches δc = 9.00 µm.
Here δ is the full face-to-face gap, and L is the added crack length at each end.
Advancing either outer crack front also consumes an intrinsic work Γ0 = 22.0 J/m²,
separate from connector work. Area means area of the crack plane, counting a pair of new faces once. Treat the
intrinsic front process as spatially negligible. The bulk outside the separated region is linear elastic; assume
symmetric, quasistatic growth and no other damage.
Following the monotonic branch from crack initiation, find: (1) the remote stress Σ, in MPa, when a connector adjacent to the original slit first fails; (2) the corresponding L, in mm per end.
Give a brief method and one physical or numerical check. Each numerical answer must be within ±0.3% of
the reference. Budget: 45 minutes; Python with NumPy and SciPy is available.
2 The physical picture
Before any formula, watch what happens as the load rises. Drag the slider, or press play. The
opening is drawn about 160 times larger than the lengths along the crack.
The oldest connector is stretched toof its breaking gap
No connectors yet: the crack has not grown.
The slit opens. At low load nothing grows: the slit opens elastically, widest in the middle.
The crack starts to grow. The fronts need only the small work Γ0 to advance, so growth
starts early, far below the final load.
Connectors stay behind and pull back. Each new piece of crack is still held by connectors. They carry part
of the load and shield the fronts. In this problem that means the load must keep rising for the crack to keep growing,
all the way to the first failure: the growth is stable.
The oldest connector is stretched most. It sits where the original slit ended, and it has been stretching
ever since the crack passed it. When its gap reaches δc, it breaks. That is the moment the
problem asks about.
So the answer needs two things at once: how much load keeps the fronts moving (the tip, step 3), and how far the
oldest connector has opened (the root, step 4). Notice also how long the bridged zones have become by the end: comparable
with the slit itself. That is why a single toughness number cannot describe this crack (step 1).
The slit opens elastically. Nothing grows yet.The fronts advance. Connectors stay behind across the new crack and stretch.The oldest connector has reached its breaking gap and fails.
3 Solve it step by step
Each step asks one question. Try it, check your number, then open the working.
If the bridged zone were much shorter than the crack, the connectors would simply add their work
σbδc to the toughness. Whether that holds depends on one material
length:
Your turn. Compute ℓ and compare it with the slit.
ℓ = mm
Show the working
E′ = 141.1 GPa, so ℓ = 7.93 mm and a/ℓ = 0.30. The slit is shorter than the
material length, so expect a bridged zone that is not small compared with the crack: large-scale bridging.
Then the load has to be computed from the body and the bridging law together. Step 5 confirms it with the solved zone length.
Keep the toughness estimate for comparison at the end:
There are two unknowns, the load Σ and the bridged length L (or the current half-length
c = a + L). So two conditions are needed at the moment the first connector fails.
Your turn. Write the two conditions in words before opening the working. Then compute
K0 = √(E′Γ0).
K0 = MPa√m
Show the working
At the front the crack advances quasistatically, so the energy reaching the tip equals
Γ0. At the other end of the bridged zone, the oldest connector, which has opened most,
reaches δc. That connector sits at the root of the original slit, x = a:
Here K0 = 1.762 MPa√m. The connectors’ work does not enter the tip condition: it is
spent behind the tip, and the tip only sees Γ0.
Remote tension on a crack with free faces is equivalent, for the tip intensity and the opening, to the same crack
with pressure on its faces. In that equivalent problem the crack of half-length c carries a pressure Σ on
the slit and Σ − σb on the bridged zones.
Your turn. Write Ktip for these pressures and apply the tip condition. As a
check, at what load does the crack start to grow (L = 0)?
Σstart = MPa
Show the working
A uniform pressure Σ on the whole crack, minus σb on a < |x| < c:
Setting Ktip = K0 (the positive root: the crack is opening) gives the load
along the growth path:
At c = a the first term vanishes and Σstart = K0/√(πa) = 20.29 MPa.
From there, in this problem, the load rises as the zone grows, because the connectors shield the tip. (With other
values it can pass a maximum first; the explorer shows such a case.)
This is the step that decides the answer, and the one where the AI agents split (Section 5).
Your turn. Find the full opening δ(a) of the crack at x = a on
the growth path of step 3. Hint: split the load into the part that gives zero tip intensity and the rest.
Show the working
Split the load of step 3:
Under ΣD together with the connectors’ traction, the tip intensity is zero. This is the
strip-yield (Dugdale) state, with σb in the place of the yield stress. Its opening at the end
of the open part is the classical result
The rest is a uniform stress on an open crack of half-length c, which opens as an ellipse; at
x = a it adds
Together:
The first term is the opening of the zero-intensity state, load and connectors together. The second is what the
front work adds.
Another route, to check an opening formula independently
Build the opening from the crack-opening Green function. For a crack |s| < c with symmetric
face pressure p(s), the full opening at x = rc is
A uniform pressure gives the ellipse 4p√(c² − x²)/E′. For
the closing traction on the bridged zones, the integral at r = a/c has a closed form:
Putting in the pressures of step 3 and the tip condition gives the same δ(a) as above.
Step 5 Solve, and check
Set δ(a) = δc. With step 3 this leaves one equation for one unknown.
Your turn. Solve it for c, then get L and Σ, and enter them in
the answer boxes.
Show the working and the answer
Write c = aeu. Then
and dividing δ(a) = δc by σba/E′ gives
with
Here ℓ/a = 3.306 and k = 0.1268. The left side rises steadily with u, so there is one
root: u = 0.9941, hence c = aeu = 6.486 mm.
L = 4.086 mm at each end and Σ = 133.7 MPa
(121.4 MPa from the connectors’ shielding plus 12.3 MPa from the front work).
Checks.
The bridged zone is 1.70 times the original half-slit: large-scale bridging, as step 1 said. The toughness
estimate, 165.4 MPa, is 24% too high.
Without front work the equation solves in closed form, the strength formula of the source paper:
From 20.29 MPa at the start, the load and the root opening both rise all the way to the failure, so the
event is reached on a rising load.
4 Explore
Move a slider and watch the two conditions meet. E, ν and
σb stay at the values of the problem. Background for the load maximum:
stability.
Try:
The problem as given.
a = 100 mm: L falls to 2.46 mm, close to the small-scale estimate of the zone (2.43 mm), and Σ comes to about 0.5% below the toughness estimate. For a long crack the bridging law condenses into a toughness.
Γ0 = 0: the load moves by 1.4%, the bridged length by 56%. The front work matters little for the strength and a lot for the size of the zone.
δc = 50 µm: the zone grows to hundreds of millimetres and the load passes a shallow maximum, 161.0 MPa at L = 240 mm, before the first connector fails. On a rising load the crack becomes unstable at that maximum.
Load at first failure
Bridged length, each end
Load along the growth path. The crack grows as the load rises, until the first connector fails.Opening at the root of the slit. The first connector fails when it reaches δc.
Common wrong answers at these values
If you…
Σ (MPa)
L (mm)
5 Find the error
Two AI agents were given this problem without the source paper. Both set up the two conditions
correctly. They differed in one relation, the opening at the root (step 4). Here is what each wrote, in the
agents’ notation: t is the connector traction σb.
Agent A
Agent B
One of them is wrong. Do not derive the right formula: test them, on two cases whose answer is known.
Test 1 · no connectors
With t = 0 the crack is an open crack under Σ, and its opening is the ellipse
(In A’s form the stress beyond ΣD is K0/√(πc); with
t = 0 that is all of Σ.)
Which formulas give the ellipse at x = a?
Test 2 · a strip-yield crack
Load the bridged crack so that the tip intensity is zero (K0 = 0, Σ = ΣD)
and take c = 2a. The textbook strip-yield opening is
Evaluate each formula there, in units of ta/E′.
A:
B:
Your verdict. Which agent wrote a wrong opening?
What happened
Test 1 passes both formulas. Test 2 separates them: the correct root opening is
(8/π) ln 2 = 1.765 ta/E′, and B’s formula gives
0.619 ta/E′. Only a test that involves the connectors can see an error in the
connectors’ term.
Agent B was DeepSeek V4.1 Flash (run with reasoning off). From the case study:
DeepSeek on the slit, with reasoning off, wrote the tip intensity correctly but took the root
opening as (4/E′)[Σ√(c² − a²) − t(c − a)],
which is not the opening of a crack under that pressure. With it, the root connector reaches δc
only at L = 34.3 mm and Σ = 158.5 MPa, 740% and 18.5% above the key. Eq. 45 gives an opening of 24.3 µm
at that state, so on the actual path the root connector had failed long before. Its opening “check”
evaluated a double integral that, at x = a, reproduces the same t(c − a) term.
It scored 47: no points for the numbers, and full verification credit for a correct, independent check of the tip
intensity.
Agent A was GLM-5.3.
GLM on the slit built the root opening itself: the opening of a strip-yield crack under the stress that gives zero tip intensity, plus
the opening of an open crack under the remaining stress K0/√(πc). That is Eq. 45 in another form. It checked the first part against a
dislocation-density integration, to 6 × 10⁻¹¹, and solved the whole problem again by a separate
spectral method, 133.70 MPa and 4.079 mm. Graded 100.
“The key” is the reference answer and “Eq. 45” the source paper’s root
opening. Grades are rubric totals out of 100 given by another AI model (Codex), not measures of accuracy; no expert has
reviewed the case. The same two agents also ran with notes about the paper, and then both got this problem right.
In the explorer above, tick “show Agent B’s formula” to see where it meets δc.
The two answers as the agents wrote them
Agent A (GLM-5.3)
By superposition (linearity in the loads) it is the
classical Dugdale CTOD at the zero-K stress
Σ_D = (2t/π)arccos(a/c) for the same (a, c), plus the
Griffith opening produced by the extra remote stress
K₀/√(πc):
δ(a) = (8ta/πE′)·ln sec θ + 4K₀√(c² − a²)/(E′√(πc)),
θ = arccos(a/c).
Agent B (DeepSeek V4.1 Flash)
**Connector failure.** The connector adjacent to the
original slit sits at x = a⁺ and has the largest gap.
Using the same superposition for the opening (full
gap) at x:
δ(x) = (4/E′)·[ (Σ − t) √(c² − x²)
+ t ( x − c + √(c² − x²) ) ],
so at the slit edge
δ(a) = (4/E′)·[ Σ √(c² − a²) − t (c − a) ].
6 Take away
A toughness needs a short zone
Here the zone at first failure is 1.7 times the half-slit, and the toughness on the original slit overestimates the load
by 24%. The finite geometry has to be solved with the law.
A check that reuses the formula cannot test it
DeepSeek’s opening check integrated an expression that reduces to its own wrong term at
x = a, so it confirmed the error. Pick a check that exercises the term you doubt.
These rest on eight runs of two agents on two problems: observations to test on new problems, not measured rates.
The full case study has the second problem, all runs and the grading.
Tell us how it went
What helped, where you got stuck, or an error you found. The button opens a pre-filled issue in the
website’s public GitHub repository, in a new tab. Your text is sent to GitHub when that tab opens and becomes
public only if you submit the issue there (a GitHub account is needed). Please do not include private information.
Nothing is stored on this page.
The problem is built on G. Bao and Z. Suo (1992), Remarks on crack-bridging concepts,
Appl. Mech. Rev. 45, 355-366; the agents did not receive the paper.
The task text: the task file of the case, problem T1.
The reference answer and the formulas of steps 3 to 5: the case’s reference script,
reference.py, which also holds the Green function of step 4. Its
answer was recomputed by three routes (case study, Section 8).
Steps 1 and 2, the numbers 1.70, 1462 J/m², 165.4 MPa and 24%, and the two lessons:
case study, Sections 1 to 3 and 9.
The agents’ formulas and the account of what happened: case study, Section 6;
their full answers, Agent A (lines 24 to 28) and
Agent B (lines 43 to 50); their grades,
A and B.
The explorer runs the reference script’s solution in your browser and is tested against it. You can also check an
answer file with the case’s own checker, in the case files.